Technical data
Phisical and mechanical parameters of Particle Boards
| Parameter | Unit | Standards EN 312, Tab. 1, Tab. 3 - Typ P2 | Testing standard |
||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thickness |
mm |
8 |
10 |
12 |
15 |
16 |
18 |
19 |
22 |
25 |
28 |
32 |
36 |
38 |
|
| Density |
kg/m3 |
720 |
700 |
690 |
670 |
660 |
650 |
650 |
640 |
640 |
620 |
610 |
610 |
600 |
EN 323 |
| Bending strenght |
N/mm2 |
11 |
11 |
11 |
11 |
11 |
11 |
11 |
10,5 |
10,5 |
9,5 |
9,5 |
8,5 |
8,5 |
EN 310 |
| Integral bond |
N/mm2 |
>0,4 |
>0,4 |
>0,4 |
>0,35 |
>0,35 |
>0,35 |
>0,35 |
>0,3 |
>0,3 |
>0,25 |
>0,2 |
>0,2 |
>0,2 |
EN 319 |
| Tearing off |
N/mm2 |
>0,8 |
EN 311 |
||||||||||||
| Swelling after 24h* |
% |
<16 |
<16 |
<16 |
<15 |
<15 |
<15 |
<15 |
<15 |
<15 |
<15 |
<15 |
<14 |
<14 |
EN 317; Norms according to EN 312, Tab.4 |
| Free formaldehyde content |
mg / 100 g.s.m. |
<8,0 |
EN 120 |
||||||||||||
| Moisture content |
% |
from 5 to 13 |
EN 322 |
||||||||||||
| Mineral particle content* |
% |
<0,3 |
Sample combustion and HCD etching method |
||||||||||||
| Thickness tolerance |
mm |
+/- 0,3 |
EN 324-1 |
||||||||||||
| Length and width tolerance |
mm |
+/-5 |
EN 324-1 |
||||||||||||
| Squareness tolerance |
mm/m |
2 |
EN 324-2 |
||||||||||||
| Edge straightness tolerance |
mm/m |
1,5 |
EN 324-2 |
||||||||||||
* Requirements are not specified for boards type P2. Tests can be done on request
Thickness and size of Particle Boards
| Size (length x width) mm | Thickness mm |
|||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| 2070 x 2620 |
- |
- |
12 |
15 |
16 |
18 |
22 |
(25)* |
28 |
- |
| 2800 x 2070 |
(8)* |
(10)* |
12 |
15 |
16 |
18 |
22 |
(25)* |
28 |
(38)* |
* on request